WoodDensity
ρ -
(kg/m3)
Fibre Stress at Elastic Limit
- σy -
(MPa)

Modulus of Elasticity
- E -
(GPa)
Compressive Strength parallel to Grain
- σ -
(MPa)
Shear Strength parallel to grain
- τ -

(MPa)
Alder, red 410 68 9.5 40.1 7.4
Ash - Black, Blue, Green, Oregon, White 490 - 600 87 - 103 9.4 - 12 41.2 - 51.1 10.8 - 14
Aspen - Bigtooth, Quaking 390 63 9.9 36.5 7.4
Baldcypress 460 73 9.9 43.9 6.9
Baswood, American 370 60 10.1 32.6 6.9
Beech, American 640 103 11.9 50.3 13.9
Birch - Paper, Sweet, Yellow 550 - 620 85 - 114 11 - 15 39.2 - 58.9 8.3 - 15.4
Butternut 380 56 8.1 36.2 8.1
Cedar - Atlantic White, Eastern Red, Incence, Northern White, Port-Orford, Western Red, Yellow 310 - 470 45 - 88 5.5 - 11.7 27.3 - 43.5 5.5 - 9.4
Cherry, black 500 85 10.3 49 11.7
Chestnut, American 430 59 8.5 36.7 7.4
Cottonwood - Balam Poplar, Black, Eastern 310 - 400 27 - 59 7.6 - 9.4 27.7 - 33.9 5.4 - 7.2
Douglas-fir - Coast, Inerior West, Interior North, Interior South 460 - 500 82 - 90 10.3 - 13.4 43.1 - 51.2 7.8 - 10.4
Elm, English 560 40 - 54 11.8 17 - 32 8 - 11.3
Elm, Dutch 560 42 - 60 7.7 18 - 32 7.2 - 10
Fir 320 - 430 61.4 - 75.8 8.9 - 11.9 33.5 - 44.2 6.2 - 8.4
Hackberry 530 76 8.2 37.5 11
Hemlock - Eastern, Mountain, Western 400 - 450 61 - 79 8.3 - 11.3 37.3 - 49 7.3 - 10.6
Hickory, pecan - Bitternut, Nutmeg, Pecan, Water 600 - 660 94 - 123 11.7 - 13.9 47.6 - 62.3 14.3
Hickory, true - Mockernut, Pignut, Shagbark, Shellbark 690 - 720 125 - 139 14.9 - 15.6 55.2 - 63.5 12 - 16.8
Honeylocust 101 11.2 51.7 15.5
Larch, Western 520 90 12.9 52.5
Locust, black 690 134 14.1 70.2 17.1
Magnolia - Cucumbertree, Southern 480 - 500 77 - 85 9.7 - 12.5 37.6 - 43.5 9.2 - 10.5
Mahogany 545 60 8.7 45 6.0
Maple - Bigleaf, Black, Red, Silver, Sugar 480 - 630 61 - 109 7.9 - 12.6 36 - 54 11.9 - 16.1
Oak, red - Black, Cherrybark, laurel, Northern Red, Pin, Scarlet, Southern Red, Water, Willow 590 - 690 75 - 125 10.3 - 13.1 42 - 60.3 9.6 - 14.3
Oak, white - Bur, Chestnut, Live, Overcup, Post, Swamp Chestnut, Swamp White, White 640 - 880 71 - 127 7.1 - 13.7 41.8 - 61.4 10.3 - 13.8
Pine - Eastern White, Jack, Loblolly, Lodgepole, Longleaf, Pitch 350 - 590 59 - 100 8.5 - 13.7 33.1 - 49.2 6.1 - 10.4
Poplar, Yellow 420 70 10.9 38.2 8.2
Sassafras 460 62 7.7 32.8 8.5
Spruce - Black, Engelmann, Red, Sitka, White, Norway 350 - 430 63 - 79 7.9 - 11 37 - 44 6.8 - 9.2
Sweetgum 520 86 11.3 43.6 11
Sycamore, American 490 69 9.8 37.1 10.1
Tupelo - Black, Water 500 66 8.3 - 8.7 38.1 - 40.8 9.2 - 11
Walnut, black 550 101 11.6 52.3 9.4
Willow, black 390 54 7 28.3 8.6

Tension Unit Converter Chart

Download and print Tension Unit Converter Chart

Panel Products

Panel Products - Mechanical Properties
PanelDensity
ρ -
(kg/m3)
Fibre Stress at Elastic Limit
- σy -
(MPa)

Modulus of Elasticity
- E -
(GPa)
Hardboard 900 - 1000 31 - 56 3.1 - 5.5
MDF - Medium Density Fiberboard 700 - 900 36 3.6
Particleboard 600 - 800 15 - 24 2.8 - 4.1
OSB - Oriented Strandboard 500 - 800 22 - 35 4.4 - 6.3
Plywood 400 - 600 34 - 43 7 - 8.6

Structural Timber Products

Structural Timber Products - Mechanical Properties
Structural TimberDensity
ρ -
(kg/m3)
Fibre Stress at Elastic Limit
- σy -
(MPa)

Modulus of Elasticity
- E -
(GPa)
Glued-laminated Timber 400 - 600 29 - 63 9 - 14.5
Laminated Veneer Lumber 400 - 700 34 - 86 9 - 19

Related Topics

  • Beams and Columns

    Deflection and stress in beams and columns, moment of inertia, section modulus and technical information.

Related Documents

Search

Search is the most efficient way to navigate the Engineering ToolBox.

Engineering ToolBox - SketchUp Extension - Online 3D modeling!

3D Engineering ToolBox Extension to SketchUp - add parametric components to your SketchUp model

Add standard and customized parametric components - like flange beams, lumbers, piping, stairs and more - to your Sketchup model with the Engineering ToolBox - SketchUp Extension - enabled for use with older versions of the amazing SketchUp Make and the newer "up to date" SketchUp Pro . Add the Engineering ToolBox extension to your SketchUp Make/Pro from the Extension Warehouse !

Translate this Page

Translate this page to Your Own Language .

About the Engineering ToolBox!

Privacy Policy

We don't collect information from our users. More about

We use a third-party to provide monetization technologies for our site. You can review their privacy and cookie policy here.

You can change your privacy settings by clicking the following button: .

Citation

This page can be cited as

  • The Engineering ToolBox (2011). Wood, Panel and Structural Timber Products - Mechanical Properties. [online] Available at: https://www.engineeringtoolbox.com/timber-mechanical-properties-d_1789.html [Accessed Day Month Year].

Modify the access date according your visit.

3D Engineering ToolBox - draw and model technical applications! 2D Engineering ToolBox - create and share online diagram drawing templates! Engineering ToolBox Apps - mobile online and offline engineering applications!

Unit Converter

















































5.16.12

.